FKM Compounding: Quick Troubleshooting Guide

FKM Compounding: Quick Troubleshooting Guide

FKM Compounding: Quick Troubleshooting Guide

Core Defects: Mold Sticking, Bubbling, High Compression Set (CS)

1. Root Cause Summary

dbab38df4949e3733ba37c19ea1cf3ad

2. Solution by Vulcanization System

A. Bisphenol AF System (most common for Type 26 & terpolymers) Focus: Moisture control & stepped heating.

51de83539ca01865911075bd72b123a9

B. Peroxide System (for G-type, low-temp, perfluoroelastomers) Focus: Oxygen exclusion & correct co-agent ratio.

02b94347041c3d852a569fb08001e25a

3. On-Site Troubleshooting Checklist (When Defects Appear)

If a batch fails, check these in order:

1. Rheometer (MDR) Data:

– Is S’min too high? → Compound scorched or hardened.

– Does T90 match your mold time? → Under-cure risk.

– Is ΔS’ (torque rise) below spec? → Low crosslink density.

2. Raw Material Moisture:

– Test Ca(OH)₂, MgO, and carbon black for moisture (loss on drying).

– Rule of thumb: If the bag feels warm or clumpy, do not use.

3. Mold Temperature Uniformity:

– Use a surface thermocouple. All cavity zones must be within ±2°C.

4. Second-Stage Oven:

– Ensure forced air circulation is working.

– Check that volatiles (HF, water) are being exhausted, not re-condensing.

Key Takeaway (One-Liners)

• Bisphenol System: “Control MgO activity, keep it dry, and use stepped post-cure.”

• Peroxide System: “Vacuum or seal the mold, balance peroxide with TAIC, and use ZnO (not lime).”

By following these specifications, you eliminate sticking and bubbling while maximizing compression set resistance and seal life.